REFLECTOR: Fastbuild Wing Delaminations

gpoole gpoole at zeta.org.au
Mon Jul 10 20:46:37 CDT 2006


Certainly is Hiroo. Some inject and then leave a broad weight on top to
ensure bonding.

 

Greg in Sydney

 

-----Original Message-----
From: reflector-bounces at tvbf.org [mailto:reflector-bounces at tvbf.org] On
Behalf Of Hiroo Umeno
Sent: Tuesday, 11 July 2006 10:49 AM
To: reflector at tvbf.org
Subject: REFLECTOR: Fastbuild Wing Delaminations

 

We were applying and sanding the "Smooth UV Primer" and discovered that our
fast build wing we got in 1999 has developed series of delamination bubbles.
Most are about 1 inch in diameter but one is about 6 inch.  Most are located
on top of the wing the near the leading-edge.

 

I have read here that the standard repair procedure is to drill a hole on
top of the bubble and inject them with epoxy, then sand smooth.  Is that
still the commonly accepted practice?

 

Hiroo

-------------- next part --------------
An HTML attachment was scrubbed...
URL: http://www.tvbf.org/mailman/private/reflector/attachments/20060711/8c3699b9/attachment.html 


More information about the Reflector mailing list